Study on Temper Embrittlement of GB 30CrMnSi Structural Steel

In metal materials, a strictly appropriate heat treatment process can endow 30CrMnSi steel with excellent properties and quality, making it widely used in multiple fields. However, GB 30CrMnSi structural steel has a tendency to temper brittleness during the tempering process (within specific temperature ranges of 250-380℃ and 460-650℃), which affects its overall performance and application scope. So, what is the root cause of temper brittleness? How to effectively prevent and improve this problem? This article will deeply discuss the temper brittleness of GB 30CrMnSi structural steel from a professional perspective to help you better understand and address this challenge.

Analysis of the Causes of Temper Brittleness

1. Low-temperature Temper Brittleness (250-380℃ Range)

When GB 30CrMnSi structural steel is tempered at 250-380℃, cementite in the quenched steel precipitates at the original austenite grain boundaries or martensite interfaces, forming flaky or network carbides. These carbides act as “crack seeds” within the steel, weakening the bonding force of grain boundaries and reducing the impact toughness of the steel, which is the main cause of low-temperature temper brittleness.

This brittleness is irreversible, and the existing embrittlement cannot be eliminated by reheating. 30CrMnSi steel contains a certain amount of silicon, which can delay the formation of cementite, thereby increasing the initial temperature of low-temperature temper brittleness. However, brittleness is still difficult to avoid.

2. High-temperature Temper Brittleness (460-650℃ Range)

When tempered at 460-650℃ or even higher temperatures, impurity elements such as phosphorus (P), antimony (Sb), and arsenic (As) in 30CrMnSi will segregate to the austenite grain boundaries. Meanwhile, alloying elements like Cr, Ni, Mn, and Si have a strong affinity with impurity elements, promoting the segregation of impurity elements at the grain boundaries. This reduces the bonding force of grain boundaries, deteriorates toughness, causes grain boundary embrittlement, significantly decreases the fracture strength of grain boundaries, and forms high-temperature temper brittleness.

This brittleness is reversible. By reheating to above 650℃ and rapidly cooling, the segregated elements can be diffused or the brittle phases can be dissolved, thereby restoring toughness. The addition of molybdenum (Mo) and rare earth elements can hinder the segregation of phosphorus and alleviate high-temperature temper brittleness.

Prevention and Improvement Measures

In the face of the temper brittleness problem of GB 30CrMnSi structural steel, the industry is not helpless. The following are some prevention and improvement measures:

(1) For low-temperature temper brittleness, try to avoid final tempering in the range of 250-380℃. A rapid tempering cooling process can be adopted to prevent carbides from precipitating in large quantities at grain boundaries, thereby avoiding a decrease in toughness. Additionally, during the composition design of 30CrMnSi alloy steel, appropriate amounts of alloying elements such as molybdenum (Mo) and tungsten (W) can be added to inhibit the precipitation of carbides.

If high hardness is required at lower temperatures, “subcritical tempering” or tempering at a temperature slightly above 380℃ can be considered, with strict control of the holding time. Moreover, replacing the traditional quenching + low-temperature tempering process with isothermal quenching can enable GB 30CrMnSi structural steel to obtain lower bainite microstructure, thereby improving impact toughness.

(2) For high-temperature temper brittleness, strictly controlling the content of impurity elements in 30CrMnSi materials is crucial. Advanced smelting processes can reduce the residual amounts of phosphorus (P), tin (Sn), antimony (Sb), etc. During tempering, adopting rapid cooling to pass through the sensitive temperature range or performing multiple tempering treatments can also effectively reduce the impact of temper brittleness.

(3) At Songshun, we continuously optimize the tempering process by adjusting the tempering temperature and holding time to avoid the brittle-sensitive intervals, thereby reducing the risk of brittleness. Post-treatment methods such as two-stage tempering, isothermal tempering, cryogenic treatment, and stress relief can also be adopted to further reduce the brittleness of the material.

(4) Controlling the composition and impurity content of GB 30CrMnSi structural steel, and selecting clean steel with extremely low impurity contents (especially P, As, Sb, Sn). Modern smelting technologies can produce high-purity steel with P content below 0.005%, and such steel shows significantly reduced sensitivity to low-temperature temper brittleness.

(5) Within the allowable range, appropriately adjust the alloy composition. For example, adding a certain amount of molybdenum (Mo) or vanadium (V) can significantly reduce the steel’s sensitivity to both first-type and second-type temper brittleness, enhancing toughness. It should be noted that although manganese (Mn) and silicon (Si) can improve strength, they may promote temper brittleness, so the advantages and disadvantages need to be weighed.

Conclusion

Although the temper brittleness problem of GB 30CrMnSi structural steel is challenging, by deeply understanding its causes and mastering effective prevention and improvement measures, we can restore the brilliance of this material. In addition to solving the temper brittleness issue, at Songshun, we also conduct research on the physical and mechanical properties of 30CrMnSi structural steel, committed to enhancing material performance, providing high-quality steel, and offering strong support for the future of the industry.