sales@songshunsteel.com
Still troubled by die edge chipping? Wondering how to double the performance of impact-resistant tool steel? The answer lies in the heat treatment process of S7 material. As an air-hardening impact-resistant tool steel, S7 gains outstanding properties through rigorous heat treatment procedures, making it highly favored across various industries. However, do you really have an in-depth understanding of the S7 steel heat treatment process? This article will give a full breakdown of the core procedure of S7 materials provided by Songshun.
The heat treatment of AISI S7 steel is not a simple process of heating, soaking and cooling, but a multi-stage synergistic metallurgical procedure.Each heat treatment step including annealing, preheating, austenitization, quenching and double tempering plays an essential role. Its heat treatment mainly involves the following key procedures:
At Songshun, our S7 tool steels are supplied in the annealed condition. Forged S7 material must first undergo the annealing process to eliminate forging hardening, soften the microstructure, and facilitate subsequent machining.
The conventional S7 spheroidizing annealing process is performed by first heating the material to 815–870°C (1500–1600°F). After soaking, cool it in the furnace to below 500°C before taking it out, then air-cool to room temperature. The final hardness is generally no more than 230 HB. This process produces a spheroidal pearlite structure, refines grain structure, greatly improves machinability, and completely relieves forging stress.
We also adopt a more efficient process at Songshun: isothermal annealing. This advanced annealing process involves heating to 810°C–870°C, rapidly cooling to 760°C for isothermal soaking for 4 hours, followed by air cooling. Isothermal annealing at 760°C can reduce the hardness to an impressive 167 HB, about 31 HB lower than isothermal annealing at 720°C. It not only greatly reduces tool wear but also creates an ideal spheroidized microstructure foundation for subsequent heat treatment.
>Special Notice: Slow cooling must be strictly implemented. Rapid cooling will result in excessive hardness and deteriorated machinability.
For AISI S7 with complex geometries, or after rough machining, welding, EDM and other processes, stress relief annealing must be performed prior to quenching. This process eliminates residual stress fields and prevents distortion or cracking caused by superimposed stresses during quenching. In service of the mold, low-temperature stress relief tempering conducted every 50,000 impacts can repair micro-damage, improve hardness retention rate, and extend service life by 60%–80%.
The standard procedure of stress relief annealing is generally heating to 649–677°C (1200–1250°F), holding at this temperature for a specified period, followed by furnace cooling to room temperature as the preferred method.
>Special Notice: Skipping this step for direct quenching may increase the scrap rate of complex geometric parts (such as molds with sharp corners and large wall thickness variations) by 3 to 5 times.
Why is preheating required? S7 material features low thermal conductivity. Direct high-temperature quenching will cause severe dimensional distortion and even cracking. This process reduces thermal shock before quenching and hardening, improves temperature uniformity, and avoids cracking or deformation induced by rapid temperature rise. Meanwhile, it is critical to protect the surface of S7 shock-resisting tool steels from decarburization.
Generally, preheating of AISI S7 round bar adopts a two-stage process:The first stage: preheat at 650–700°C and hold until the temperature of the workpiece becomes uniform internally and externally;The second stage: preheat at 780–870°C, with the holding time set to half of the austenitization holding time.
>Special Notice: The heating rate must be strictly controlled during preheating to prevent internal cracks in the material caused by excessive temperature difference.
Austenitization is the key procedure to achieve high hardness. Heat ASTM A681 S7 tool steel to its austenitization temperature range to fully dissolve internal carbides and completely transform the microstructure into austenite, laying a foundation for the subsequent quenching process.
The typical austenitization temperature range for this steel is 925–955°C (1697–1751°F), followed by air quenching or oil quenching after temperature holding.
>Special Notice: Overheating or overburning must be avoided; otherwise, coarse grain structure will be formed and the toughness of S7 material will be impaired. The holding time shall be adjusted according to the size and shape of the workpiece to ensure full austenitization inside the material.
S7 steel quenching is the core procedure of heat treatment. It mainly transforms austenite into martensite through rapid cooling, so as to remarkably enhance the hardness and strength of the material.
S7 material is an air-hardenable steel. Its greatest advantage lies in that it generates extremely minimal distortion during quenching when compared with oil-quenched or water-quenched steel grades. The quenching method is determined by the cross-sectional size and distortion sensitivity of the workpiece:
| Workpiece Cross-section | Recommended Quenching Method | Target Cooling Temperature |
|---|---|---|
| ≤63.5 mm (2.5 inches) | Still Air Quenching | 66–51°C (150–125°F) |
| 63.5–152.4 mm (2.5–6 inches) | Pressurized Gas Quenching / Interrupted Oil Quenching(Oil quench until darkening ≈ 482°C, then switch to air cooling) | 66°C |
| >152.4 mm (6 inches) | Full Oil Quench to 150°F, temper immediately | 66°C |
>Special Notice: Oxidation and decarburization on the workpiece surface shall be avoided during quenching. Heating can be performed under a protective atmosphere or in a vacuum environment.
After quenching, S7 material shall be tempered immediately. The main purposes are to relieve quenching stress, balance hardness and toughness, while maintaining high hardness and stable microstructure.
ASTM S7 steel must undergo double tempering (minimum soaking time of 2 hours per tempering cycle; air cool to room temperature between the two tempering cycles). The specific tempering temperature and holding time shall be adjusted according to actual application requirements:
| Tempering Type | Temperature Range | Hardness Range | Key Characteristics | Ideal Application Fields |
|---|---|---|---|---|
| Low Temperature Tempering | 200–260°C | 55–62 HRC | Maximum hardness and wear resistance with moderate toughness | Precision blanking dies, blanking punches, chisels |
| Medium Temperature Tempering | 450–520°C | 54–58 HRC | Optimal balance of hardness and toughness | Cold heading dies, forming tools |
| High Temperature Tempering | 570–650°C | 50–54 HRC | Highest impact toughness and good hot hardness | Forging dies, heavy-duty impact tools, pneumatic tools |
>Special Notice: Regardless of the selected temperature, multiple tempering (2–3 cycles) is strongly recommended with a soaking time of no less than 2 hours each time, to completely eliminate retained austenite and internal quenching residual stress.
A: Not recommended. S7 steel plate is an air-hardenable steel. Water quenching will generate excessive internal stress and cause cracking easily. Water-oil dual-medium quenching may only be considered for workpieces with extremely large cross-sections and low requirements on distortion control.
A: Mandatory. Stress relief annealing shall be performed immediately after welding, followed by re-quenching and re-tempering. Direct service without post-weld treatment will result in cracking at the weld zone.
A: Absolutely not. Quenched S7 steel is in a high-stress state with extremely high hardness but severe brittleness; even minor impact may lead to fracture. Tempering must be conducted immediately after quenching.
A: Yes. The chromium and molybdenum composition of S7 material is highly suitable for liquid carburizing and gas nitriding, which can greatly improve surface hardness and wear resistance.
In addition to the above core heat treatment processes for S7 steel, Songshun can also adopt special heat treatment processes such as cryogenic treatment, surface nitriding and vacuum heat treatment to further upgrade S7 performance. At Songshun, we are well aware that heat treatment processes exert a vital influence on the properties of ASTM S7 material. For this reason, we strictly control every detail in the heat treatment process of AISI S7 material, and commit ourselves to producing high-quality materials to provide reliable guarantee for your applications.

Welcome to contact us at any time through the following ways