sales@songshunsteel.com
DIN XPM material is a kind of pre-hardened plastic mold steel of Cr-Ni-Mo alloy. Its microstructure can be optimized through a rigorous heat treatment process, while it also boasts comprehensive performance advantages such as high toughness, excellent machinability and superior polishing effect. However, a slight deviation in the heat treatment parameters of DIN XPM tool steel bar or inadequate control over the details of certain process steps may bring about various challenges, directly leading to mold deformation, cracking and other defects, which will adversely affect the product qualification rate and production costs. This is exactly why a well-known saying prevails in the industry: “Quality steel requires sophisticated processing, and the true value of XPM lies entirely in heat treatment”. Today, we will analyze the core problems, causes and corresponding solutions in the heat treatment process of DIN XPM steel from a professional perspective, help you steer clear of process “pitfalls” and produce high-quality steel products with optimal performance!
1.1 Problem:Longitudinal cracks, transverse cracks, network cracks, arc cracks and other forms appear on DIN XPM tool steel bars after quenching, most of which are found after cooling or during the tempering process.
1.2 Cause Analysis:
(1) XPM tool steel has a high content of carbon and alloying elements with a low Ms point. The stress generated by structural transformation during quenching is relatively large, resulting in a naturally higher quenching cracking tendency than ordinary steel.
(2) Rapid heating leads to an excessive temperature difference between the surface and the core of the steel bar, causing intense thermal stress due to uneven thermal expansion; or the heating temperature is too high, exceeding the material’s phase transformation point, which results in coarse grains, reduced steel toughness and increased cracking risk. Insufficient preheating will lead to a huge thermal gradient during subsequent heating, causing the accumulation of internal stress.
(3) Excessively fast cooling rate, especially the failure to achieve slow cooling in the Ms-Mf temperature range, leads to a sharp increase in phase transformation stress; or the cooling rate of the selected cooling medium exceeds the critical quenching cooling rate of the steel; alternatively, an inappropriate quenching medium is used.
(4)The presence of low-melting point harmful impurities such as S and P in the steel, or the existence of microcracks, carbide segregation and other defects. These defects will become stress concentration points and induce cracking during the heat treatment process.
1.3 Solutions:
(1) Optimize the heating process and adopt a step-by-step heating strategy. Conduct two preheating stages first to ensure uniform temperature inside and outside the DIN XPM tool steel bars, avoid abrupt changes in thermal stress, and then raise the temperature to the target austenitizing temperature (the specific temperature shall be adjusted according to the steel bar specifications) to eliminate thermal stress caused by rapid heating. Meanwhile, strictly control the heating temperature to avoid overheating; a microcomputer temperature control instrument can be adopted to ensure the temperature control accuracy reaches ±1.5℃.
(2) Select the cooling medium and method scientifically, obtain an appropriate cooling rate by adjusting its concentration ratio, and effectively reduce the phase transformation stress. For large-size steel bars, marquenching or austempering can be adopted to further reduce stress concentration.
(3) Implement strict raw material inspection, conduct a comprehensive inspection of XPM steel bars upon warehousing, focusing on the detection of harmful impurity content, carbide distribution and internal defects, and resolutely reject unqualified raw materials for production. Prioritize steel produced by vacuum smelting and secondary refining to improve material purity.
(4)Perform timely tempering treatment, send the steel bars into the furnace for tempering immediately after quenching to eliminate part of the quenching internal stress.
2.1 Problem: Inspection after heat treatment shows that the surface hardness of DIN XPM steel bar meets the standard, but the core hardness is insufficient; or there is a large hardness variation at different positions of the same steel bar. This will directly lead to reduced wear resistance and shortened service life of the products, which are prone to failure under high-load working conditions. In addition, there are also issues such as high surface hardness with a soft core, or local occurrence of soft spots and hard spots.
2.2 Cause Analysis:
(1) Inadequate austenitization at the core of large-diameter steel bars, caused by excessively low heating temperature or insufficient holding time, results in incomplete dissolution of carbides in the steel and insufficient content of carbon and alloying elements in austenite. Thus, enough martensite structure cannot be formed after quenching, leading to naturally low hardness.
(2) Excessively high tempering temperature that exceeds the reasonable range, or inadequate tempering process with insufficient secondary tempering performed, results in incomplete transformation of retained austenite.
(3)Incomplete cooling: during the quenching and cooling process, insufficient or uneven cooling rate causes part of the supercooled austenite to transform into soft structures such as pearlite and bainite instead of martensite, which impairs the overall hardness.
2.3 Solutions:
(1) Precisely control the austenitization parameters, and determine the reasonable heating temperature and holding time according to the material characteristics and effective thickness of DIN XPM tool steel bar.
(2) Strictly control the tempering temperature, select the appropriate tempering temperature according to the required hardness specification, and avoid over-temperature tempering.
(3) Optimize the cooling process to ensure the temperature uniformity and fluidity of the cooling medium, and avoid an excessive difference in cooling rate between the surface and the core of the steel bar. For steel bars with complex shapes or large dimensions, an agitating device can be adopted to improve cooling uniformity.
3.1 Problem: If DIN XPM tool steel bar suffer from deformation issues such as bending, torsion and ovality after heat treatment, and the deformation exceeds the allowable range, it will increase the difficulty of subsequent machining and even render the bars unusable.
3.2 Cause Analysis:
(1) Uneven stress distribution: inconsistent temperature changes in different parts of the steel bar during heating or cooling lead to uneven distribution of thermal stress and phase transformation stress, which induces deformation.
(2) Inhomogeneous raw material structure: problems such as carbide segregation and uneven grain size in the steel will cause asynchronous structural transformation in different regions during heat treatment, resulting in uneven volume change and thus leading to deformation.
(3) Improper furnace charging method: uneven placement, over-dense stacking of steel bars during charging, or excessive contact with furnace walls and fixtures will cause uneven stress during heating and cooling, exacerbating deformation.
(4) Variation in cooling rate: inconsistent cooling rates in different parts generate structural stress.
3.3 Solutions:
(1) Optimize the heating and cooling process to ensure uniform temperature change in all parts of the steel bar, and reduce the generation of uneven thermal stress and phase transformation stress from the source.
(2) Adopt a reasonable furnace charging method to ensure the steel bars are placed flat with uniform spacing, and avoid over-dense stacking.
(3) Conduct stress relief annealing: perform stress relief annealing on rough-machined steel bars before the final heat treatment to eliminate machining stress and reduce subsequent heat treatment deformation.
(4) Control the cooling rate: adopt mild cooling methods such as marquenching and austempering to reduce the difference between thermal stress and phase transformation stress and lower the risk of deformation. Meanwhile, prevent the steel bars from being subjected to external force interference during the cooling process.
After hardening, DIN XPM tool steel features high hardness but also high brittleness, along with considerable residual internal stress. The tempering process involves reheating the steel and controlling its cooling to eliminate residual stress, reduce brittleness, and adjust the balance between hardness and toughness—endowing the steel with sufficient hardness as well as excellent impact resistance.
A minimum of two tempering cycles is required, with three cycles recommended, since a single tempering cycle cannot fully eliminate quenching-induced stress. The first tempering cycle primarily serves to relieve quenching stress; the second stabilizes the microstructure; the third further enhances dimensional stability. For molds requiring extremely high dimensional stability, a sub-zero treatment at a temperature ranging from -80°C to -120°C can be implemented between tempering cycles.
In addition to the above issues, DIN XPM tool steel bar may encounter other challenges during the heat treatment process, which call for tailored solutions in a timely manner. Therefore, at Songshun, we exercise stringent control over the heat treatment process of DIN XPM tool steel. Only by preventing and resolving problems from the root cause and attending to every detail with meticulous care can the excellent performance of the steel be fully exerted, enabling us to provide you with high-quality materials.

Welcome to contact us at any time through the following ways