Songshun Steel & TOP Steel Manufacturer Supplier in China

H13 Nitriding Standard Process Flow: A Complete Technical Guide from Pre‑Treatment and Nitriding to Quality Inspection

Why, for the same H13 hot-work die steel, can some die‑casting molds operate stably for over 100,000 shots, while others develop thermal cracking, aluminum sticking and excessive wear after only several thousand shots? The answer often lies in the process details of H13 nitriding. As the core surface‑strengthening process for H13, nitriding directly governs the mold’s surface hardness, wear resistance, thermal‑fatigue life and other key properties. But are you really doing it correctly? This article systematically breaks down the standard process flow for H13 nitriding treatment in full detail.

Ⅰ. What is H13 Nitriding and Why Perform It?


The AISI H13 hot-work die steel nitriding treatment includes gas nitriding, ion nitriding, salt‑bath / liquid nitriding and other variants. These processes allow active nitrogen atoms to penetrate the steel’s surface layer and form a high‑hardness nitride layer to achieve surface strengthening.

After nitriding, H13 material achieves extremely high wear resistance and anti‑adhesion performance, a sharp rise in surface hardness, excellent thermal‑fatigue resistance, dimensional stability and corrosion resistance, among other benefits.

Ⅱ. Comparison of Mainstream Process Routes for H13 Nitriding Treatment


At present, there are three major technical routes for H13 nitriding in industry, each suited for different mold service conditions:

Process TypeNitrogen Source MediumTypical TemperatureCore AdvantagesApplication Scenarios
Gas NitridingAmmonia (NH₃)500–540 °CUniform nitrided layer, low equipment cost, suitable for mass productionFull nitriding of large-and medium-size die-casting molds and extrusion dies
Ion Nitriding (Plasma Nitriding)N₂+H₂ Mixed Gas450–550 °CMinimal distortion, controllable nitrided layer, local antinitriding availablePrecision complex molds, thin-wall components, anti-nitriding for threaded sections, mirror-surface molds, high-value molds
Salt-Bath Nitriding (QPQ)Cyanate Molten Salt520–580 °CFast processing speed, anti-rust capabilitySmall-size molds, standard parts such as ejector pins and sleeve ejectors

Ⅲ. Standard Process Flow for H13 Nitriding


For the vast majority of AISI H13 hot-work tool steel, gas nitriding and ion nitriding are the mainstream options. Among them, the two-stage gas nitriding process is widely recognized as the standard for H13 nitriding treatment. The following section fully dissects the complete process centered on two-stage gas nitriding.

Step 1: Pre-nitriding Pretreatment

This is the primary checkpoint that determines nitrided layer quality. The following preparations must be completed prior to H13 nitriding:

(1) Base Material Heat Treatment
Nitriding is a low-temperature surface treatment that does not change the microstructure or hardness of the base material. Therefore, AISI H13 steel heat treatment is indispensable. Quenching and tempering must be completed beforehand, and the tempering temperature must be at least 20–50 °C higher than the nitriding temperature, so as to prevent softening and distortion of the base material during nitriding.

  • Quenching: Heat AISI H13 to 1020–1050 °C for holding, followed by oil quenching or interrupted quenching.
  • Recommended pre-nitriding tempering temperature: 560–600 °C, double tempering to eliminate retained austenite and obtain uniform tempered sorbite.
  • Base material hardness control: 44–48 HRC.
  • Retained austenite content: controlled below 5 % to avoid abnormal volume expansion after nitriding.

(2) Surface Cleaning Treatment

  • Thoroughly remove machining oil, rust, decarburized layer, scale and other contaminants. Ultrasonic degreasing + blasting/polishing + solvent cleaning is recommended to guarantee uniform penetration of nitrogen atoms.
  • Recommended surface roughness: Ra ≤ 1.6 μm. Insufficient surface finish causes uneven nucleation of nitrides.
  • Residues of silicon-containing sealants or paints are forbidden, as they lead to local insufficient nitriding.

(3) Anti-nitriding Protection

  • Protect non-nitriding areas such as fitting surfaces, threaded holes and corners that do not require hardening via tin plating, anti-nitriding coating or mechanical shielding. This avoids assembly jamming caused by dimensional growth after nitriding.

Step 2: Furnace Loading and Atmosphere Purge

(1) Place the H13 tool steel workpieces inside the nitriding furnace and seal the furnace cover.

(2) After furnace sealing, exhaust must be completed before heating up to 150 °C. Introduce ammonia or nitrogen for atmosphere purge to remove air and oxygen and prevent surface oxidation. This step is critical to avoid surface oxidation of H13 steel.

(3) Purge the furnace with nitrogen (N₂) or ammonia (NH₃) to ensure the oxygen content falls below the safety threshold.

Quality Control Key Points: Excessively high oxygen content inside the furnace will cause blue-tinted oxidation on workpiece surfaces, hinder effective penetration of nitrogen atoms, and directly result in defects such as insufficient hardness and mottled discoloration. Adequate gaps between workpieces shall be reserved for gas flow passages to avoid shielding-induced case-depth non-uniformity. Ensure uniform circulation of ammonia (NH₃) to prevent “bright-dark surface” defects.

Step 3: Heating-up and Preheating Stage

Rapid heating is not desirable for H13 nitriding. H13 molds are generally large-sized with uneven wall thickness. Fast temperature rise generates significant thermal stress and leads to excessive mold distortion. A segmented heating profile is adopted as the standard heating schedule:

  • Apply stepped heating and control the heating rate (e.g. 50-100 °C/hour). Hold for soaking when approaching the nitriding temperature to ensure temperature consistency between the workpiece core and surface.
  • Introduce a small amount of ammonia throughout the whole process to maintain positive furnace pressure and prevent air infiltration.
  • Continuously monitor both furnace temperature and actual workpiece temperature.

Step 4: Boost Diffusion Stage

When the furnace reaches the preset nitriding temperature, the process enters the first phase — the boost diffusion stage.

  • Gas supply: Evacuate the furnace to below 10 Pa first, then feed mixed gas of nitrogen and hydrogen at a ratio of 1:3
  • Temperature: 510–530 °C (optimal boost-diffusion temperature for H13 steel; excessive temperature causes nitride coarsening)
  • Ammonia dissociation rate: controlled at 20-30 % (high nitrogen-potential environment)
  • Furnace pressure: 10-15 kPa gauge pressure
  • Duration: 4-10 hours (adjust according to target case depth)

The core objective of this stage is to rapidly form a dense ε-Fe₃N compound layer (i.e. white layer) on the workpiece surface, while nitrogen atoms start diffusing inwards. For H13 die-casting molds, the thickness of the white layer must be strictly controlled. An overly thick white layer increases brittleness and tends to spall during service; an excessively thin white layer delivers insufficient wear resistance and anti-aluminum-sticking performance.

Step 5: Diffusion Stage

Upon completion of boost diffusion for H13, the process proceeds to the second phase — the diffusion stage. This critical step determines the overall case depth and toughness of the nitrided layer.

  • Temperature: raise to 530-540 °C (accelerate inward diffusion of nitrogen atoms)
  • Ammonia dissociation rate: increased to 40-60 % (reduce nitrogen potential to avoid excessive nitrogen concentration on the surface)
  • Duration: 6-10 hours

By lowering the surface nitrogen concentration gradient, the diffusion stage drives continuous migration of nitrogen atoms toward the substrate, generating a thick diffusion layer with rational gradient and reducing the thickness of brittle white layer. The diffusion layer features a gentle hardness gradient and balances hardness and toughness. It serves as the main structure to resist thermal fatigue and withstand wear. For H13 nitriding, higher hardness does not equal better performance, nor does a thicker white layer. What die-casting molds and hot forging dies truly require is a gradient microstructure featuring “wear-resistant surface and tough subsurface”.

Step 6: Furnace Cooling

Opening the furnace for air cooling or oil cooling right after nitriding is strictly prohibited. Controlled slow cooling inside the furnace must be performed:

  • Stop heating and cool down at a rate of 30-50 °C/h
  • Maintain positive protective pressure by feeding a small flow of ammonia or nitrogen throughout cooling
  • Discontinue ammonia supply and switch to pure nitrogen for protection
  • Do not take workpieces out for air cooling until furnace temperature drops below 200 °C
  • Water quenching or abrupt air cooling is forbidden to avoid nitrided-layer cracking and distortion
  • Minor surface oxide film after discharging can be lightly polished; take care not to grind through the white layer.

Slow cooling serves two purposes: first, prevent mold distortion and nitrided-layer cracking induced by thermal stress; second, avoid surface oxidation and discoloration caused by high-temperature discharging, minimize dimensional variation, and preserve appearance and subsequent service performance.

Step 7: Post-Treatment and Quality Inspection

After H13 workpieces are discharged from the nitriding furnace, final inspection and necessary post-treatment shall be carried out: visual inspection, hardness test, case-depth measurement, dimensional check, metallographic examination (white-layer thickness), etc.

Posttreatments such as polishing or deburring may be performed upon requirements to guarantee service performance and surface quality of molds. If high surface finish is required, final machining should normally be completed before nitriding. Only light polishing is allowed after nitriding to prevent excessive grinding from damaging the effective nitrided layer.

Ⅳ. FAQs About H13 Nitriding Process


Q1: What is the optimal nitriding temperature for H13?

A: The standard temperature range for H13 nitriding is 500–540 °C. For the widely-adopted two-stage process in production, the boost-diffusion stage runs at 510–525 °C and the diffusion stage at 530–540 °C. Maximum surface hardness can be achieved at approximately 520 °C. Temperatures above 550 °C will cause nitride coarsening and result in reduced hardness instead.

Q2: Why is tempering required prior to ASTM H13 nitriding treatment?

A: Nitriding takes place above 500 °C. If the base-material tempering temperature is lower than the nitriding temperature, secondary tempering softening will occur in the substrate during nitriding, leading to hardness drop. Therefore, the pre-nitriding tempering temperature for H13 must be 30-50 °C higher than the nitriding temperature, typically 560-600 °C. Unrelieved residual stress will trigger nitriding distortion, dimensional instability and even locally low hardness.

Q3: How to deal with black and rough surfaces after H13 nitriding?

A: This issue may stem from oxygen leakage inside the furnace or incomplete degreasing on workpiece surfaces. It is necessary to inspect furnace sealing performance and add blasting plus acetone cleaning procedures before nitriding.

Q4: Is a deeper nitrided case depth always better for H13?

A: No. Excessively deep case depth degrades thermal-fatigue resistance and raises brittleness risk. The key lies in the matching between case depth and white-layer thickness.

Ⅴ. Conclusion


Although H13 nitriding appears to be merely one heat‑treatment procedure, every step exerts an impact on the final service life of molds. From strict pre‑treatment checks and precise two‑stage nitrogen‑potential control, to slow‑cooling distortion management and final inspection & acceptance, we rigorously control every detail throughout each phase of AISI H13 nitriding. This helps extend the service life of H13 molds by more than 2 times and cut overall manufacturing costs by over 30%.

Songshun Mold Steel provides long‑term and stable supply of H13 (4Cr5MoSiV1 / 1.2344) steel, with additional support for machining and customization. Feel free to contact us for your steel procurement requirements!

Related Articles


Songshun Steel-Logo

Dongguan Songshun Mould Steel Co., Ltd.

Welcome to contact us at any time through the following ways
Or you can email directly to  sales@songshunsteel.com